Search result: GB/T 15180-2025 (GB/T 15180-2010 Older version)
Standard ID | Contents [version] | USD | STEP2 | [PDF] delivered in | Standard Title (Description) | Status | PDF |
GB/T 15180-2025 | English | 129 |
Add to Cart
|
3 days [Need to translate]
|
Petroleum asphalts for heavy traffic road
| Valid |
GB/T 15180-2025
|
GB/T 15180-2010 | English | 149 |
Add to Cart
|
2 days [Need to translate]
|
Petroleum asphalts for heavy traffic road pavement
| Valid |
GB/T 15180-2010
|
GB/T 15180-2000 | English | 199 |
Add to Cart
|
2 days [Need to translate]
|
Petroleum asphalts for heavy traffic road pavement
| Obsolete |
GB/T 15180-2000
|
GB/T 15180-1994 | English | RFQ |
ASK
|
3 days [Need to translate]
|
Paving asphalt
| Obsolete |
GB/T 15180-1994
|
Standard ID | GB/T 15180-2025 (GB/T15180-2025) | Description (Translated English) | Petroleum asphalts for heavy traffic road | Sector / Industry | National Standard (Recommended) | Classification of Chinese Standard | E43 | Classification of International Standard | 75.140 | Word Count Estimation | 6,640 | Date of Issue | 2025-02-28 | Date of Implementation | 2025-09-01 | Issuing agency(ies) | State Administration for Market Regulation, National Standardization Administration |
GB/T 15180-2025.Petroleum asphalt for heavy traffic roads
GB/T 15180-2025 English version. Petroleum asphalts for heavy traffic road
ICS 75.140
CCSE43
National Standard of the People's Republic of China
Replace GB/T 15180-2010
Heavy traffic road asphalt
Released on 2025-02-28
2025-09-01 Implementation
State Administration for Market Regulation
The National Standardization Administration issued
Preface
This document is in accordance with the provisions of GB/T 1.1-2020 "Guidelines for standardization work Part 1.Structure and drafting rules for standardization documents"
Drafting.
This document replaces GB/T 15180-2010 "Petroleum Asphalt for Heavy Traffic Roads". Compared with GB/T 15180-2010, except for the structural adjustment
In addition to editorial changes, the main technical changes are as follows.
a) The AH-30 grade and its technical requirements were deleted (see Table 1 of the.2010 edition);
b) Added AH-170 grade and its technical requirements (see Table 1);
c) Changed the elongation of the residue at 15°C after the AH-50 film oven test, and changed the reported value to no less than 5 cm (see Table 1,
Table 1 of the.2010 edition);
d) The limit value of mass change in the film oven test has been changed (see Table 1, Table 1 of the.2010 edition);
e) Added inspection rules (see Chapter 6).
Please note that some of the contents of this document may involve patents. The issuing organization of this document does not assume the responsibility for identifying patents.
This document is proposed and coordinated by the National Technical Committee for Standardization of Petroleum Products and Lubricants (SAC/TC280).
This document was drafted by. China University of Petroleum (East China), Foshan Jiaotong Tiannuo (Guangdong) Materials Co., Ltd., Ministry of Transport Highway Research Institute
Institute, Sinopec Petrochemical Research Institute Co., Ltd., China National Offshore Oil Corporation, PetroChina Fuel Oil Co., Ltd., Beijing
Municipal Road and Bridge Building Materials Group Co., Ltd., Sinopec Qilu Petrochemical Company, Sinopec Zhenhai Refining and Chemical Company, PetroChina Liaohe Petrochemical Company,
PetroChina Karamay Petrochemical Co., Ltd., Henan Yellow River Expressway Co., Ltd., CCCC Second Highway Engineering Bureau Co., Ltd.,
Harbin Institute of Technology.
The main drafters of this document are. Zhang Yuzhen, Zeng Guodong, Guo Ning, Yan Erhu, Wang Cuihong, Wang Jinfeng, Shi Jingtao, Liu Hao, Sun Xianju, Zhang Xiaoyan,
Cao Pengyun, Lin Xixiong, Zhao Zhigang, Xue Cheng, Li Hao, Tan Yiqiu.
This document was first issued in.1994, revised for the first time in.2000, revised for the second time in.2010, and this is the third revision.
Heavy traffic road asphalt
Warning. If appropriate precautions are not followed, the products covered by this document may be at risk during production, storage, transportation and use.
This document is not intended to provide advice on all safety issues associated with this product. It is the user's responsibility to establish appropriate
safety and protection measures and determine the applicability of relevant regulatory limitations.
1 Scope
This document specifies the technical requirements and test methods for petroleum asphalt suitable for heavy traffic road construction, which is produced from petroleum as raw material through appropriate processes.
Inspection methods, inspection rules, as well as packaging, marking, storage, transportation and delivery acceptance.
This document applies to the production, sale and use of heavy traffic road petroleum asphalt in road construction projects.
2 Normative references
The contents of the following documents constitute essential clauses of this document through normative references in this document.
For referenced documents without a date, only the version corresponding to that date applies to this document; for referenced documents without a date, the latest version (including all amendments) applies to
This document.
GB/T 267 Determination of flash point and fire point of petroleum products (open cup method)
GB/T 4507 Determination of asphalt softening point - Ring and ball method
GB/T 4508 Asphalt ductility test method
GB/T 4509 Asphalt penetration test method
GB/T 5304 Petroleum asphalt film oven test method
GB/T 8928 Determination of density of solid and semi-solid petroleum asphalt
GB/T 11147 Asphalt sampling method
GB/T 11148 Determination of solubility of petroleum asphalt
NB/SH/T 0164 Rules for packaging, storage, transportation and delivery acceptance of petroleum and related products
NB/SH/T 0425 Determination of wax content in petroleum asphalt
3 Terms and definitions
There are no terms or definitions that require definition in this document.
4 Product Categories
Heavy traffic road petroleum asphalt is divided into six types according to the needle penetration range. AH-170, AH-130, AH-110, AH-90, AH-70, AH-50
Brand.
5 Technical requirements and test methods
The technical requirements and test methods for heavy traffic road petroleum asphalt shall comply with the provisions of Table 1.
......
GB/T 15180-2010
Petroleum asphalts for heavy traffic road pavement
ICS 75.140
E43
National Standards of People's Republic of China
Replacing GB/T 15180-2000
Heavy traffic road asphalt
Issued on. 2011-01-10
2011-05-01 implementation
Administration of Quality Supervision, Inspection and Quarantine of People's Republic of China
Standardization Administration of China released
Foreword
This standard JISK2207.1996 "Asphalt" (in English) the consistency of non-equivalent.
This standard JISK2207.1996 Main Differences "asphalt" as follows.
--- The increase in Chapter 2 standard normative references;
--- The standard of various grades of asphalt increased wax content not more than 3.0% of the technical requirements (Chapter 4 of this edition);
--- The standard evaporation test canceled and the associated mass change and penetration ratio indicators (see JISK2207.1996 in
Chapter 5);
--- The standard AH-5015 ℃ by the ductility of not less than 10cm to not less than 80cm (see Chapter 4 of this edition, JISK2207.
Chapter 5, 1996);
--- This standard increases the ductility of the film after 15 ℃ oven (see Chapter 4 of this edition, JISK2207. Chapter 5, 1996);
--- This standard is not less than 15 ℃ density 1.000g/cm3 modify reports 25 ℃ density (see Chapter 4 of this edition,
Chapter 5 1996). JISK2207.
This standard replaces GB/T 15180-2000 "heavy traffic road asphalt."
This standard and GB/T 15180-2000 main differences are as follows.
--- This standard canceled the extension of the film before and after the oven at 25 ℃ (see GB/T 15180-2000 in Chapter 4);
--- This standard value after the film oven test report ductility at 15 ℃ was changed to a specific value (see Chapter 4 of this edition, GB/T 15180-
Chapter 4 in 2000);
--- This standard increases the AH-30 grades and technical requirements (see Chapter 4 of this edition).
This standard was proposed by the Technical Committee of Standardization petroleum products and lubricants.
This standard by the National Standardization Technical Committee lubricant oil asphalt petroleum products and the Technical Committee.
This standard was drafted. China University of Petroleum (East China) Heavy Oil Research Institute.
The main drafters. Zhang Yuzhen, Zhang Xiaoying.
This standard replaces the standards previously issued as follows.
--- GB/T 15180-1994, GB/T 15180-2000.
Heavy traffic road asphalt
1 Scope
This standard specifies the oil as raw material, appropriate technology, the technical requirements applicable to the construction of heavy traffic road asphalt and petroleum
Test methods, as well as packaging, labeling, storage, transport and other requirements.
This standard applies to the construction of highways, highway and expressway, trunk road and other heavy traffic road asphalt, will also apply to
He each grade highways, urban roads, airport pavement, as well as emulsified asphalt, cutback asphalt and modified asphalt bitumen feedstock.
2 Normative references
The following documents contain provisions which, through reference in this standard and become the standard terms. For dated references, subsequent
Amendments (not including errata content) or revisions do not apply to this standard, however, encourage the parties to the agreement are based on research
Whether the latest versions of these documents. For undated reference documents, the latest versions apply to this standard.
GB/T 267 Petroleum products - Determination of flash and fire (Open cup)
GB/T 4507 Determination of softening point (R & B)
GB/T 4508 Determination of asphalt ductility
GB/T 4509 asphalt penetration assay
GB/T 5304 Asphalt Thin Film Oven Test Method
GB/T 8928 solid and semi-solid petroleum asphalt densitometry
GB/T 11147 bitumen sampling
GB/T 11148 asphalt solubility assay
SH/T 0425 Determination of wax content of asphalt
SH0164 petroleum product packaging, storage and delivery acceptance rules
3 Product Categories
This standard penetration range is divided into AH-130, AH-110, AH-90, AH-70, AH-50, AH-30 six grades.
4 technical requirements and test methods
The standard technical requirements and test methods are shown in Table 1.
Table 1 heavy traffic road asphalt technical requirements
project
Quality Index
AH-130 AH-110 AH-90 AH-70 AH-50 AH-30
experiment method
Penetration (25 ℃, 100g, 5s)
1/10mm
120 ~ 140 100 ~ 120 80 ~ 100 60 ~ 80 40 ~ 60 20 ~ 40 GB/T 4509
Ductility (15 ℃)/cm is not less than 10,010,010,010,080 report a GB/T 4508
Softening point/℃ 38 ~ 51 40 ~ 53 42 ~ 55 44 ~ 57 45 ~ 58 50 ~ 65 GB/T 4507
Solubility /% not less than 99.0 99.0 99.0 99.0 99.0 99.0 GB/T 11148
Flash point/℃ no less than 230 260 GB/T 267
Density (25 ℃)/(kg/m3) report GB/T 8928
......
|